Applicable materials:Lead-zinc-silver ore
Processing capacity:100tpd
1. Project Overview
Processing scale: 100 tons of raw ore/day, 24h three-shift continuous production, annual production of 300 days, annual processing of about 30,000 tons of ore;
Main products: lead-silver concentrate, zinc concentrate;
The mainstream route of the process: priority flotation (floating lead and silver first, then zinc), which is the most mature solution for small and medium-sized lead, zinc and silver mines;
2. Complete process flow
1. Crushing and screening section
Raw ore → Raw ore bin → Vibrating feeder → Jaw crusher coarse crushing → Belt conveying → Cone crusher fine crushing → Vibrating screen closed-circuit screening; the large pieces on the screen are returned to the cone crusher for re-crushing, and the qualified particles (-10~15mm) under the screen are sent to the fine ore bin.
Crushing, screening, sealed transfer points + bag dust removal to control dust.
2. Grinding and grading section
Powder ore silo quantitative feeding → Two-stage ball mill + hydrocyclone grinding; grinding fineness is conventionally controlled -0.074mm, accounting for 75% to 85%, to achieve monomer dissociation of lead, zinc, and silver minerals; qualified slurry overflows from the cyclone and flows into the flotation process.
Grinding is the section with the highest energy consumption, and the fineness directly determines the recovery rate of silver and lead.
3. Flotation process section (core process: priority flotation)
Lead-silver flotation: The slurry enters the stirring tank, and zinc inhibitors (zinc sulfate, etc.), selective collectors, and foaming agents are added; the process of one rough selection, two sweeps, and 2 to 3 selections is used to prioritize the floating of galena and associated silver minerals to obtain lead-silver concentrate; most of the silver floats up with the lead minerals and is enriched in the lead concentrate, which is the main way to recover silver.
Zinc flotation: The lead flotation tailings enter the zinc flotation mixing tank, add copper sulfate to activate the sphalerite, add zinc collector and foaming agent, and perform the same roughing + sweeping + selection to float out the zinc concentrate.
The flotation ore is gradually returned to the closed circuit to reduce metal loss; the alkali-free flotation process can be used to reduce the amount of lime and reduce the inhibition loss of silver, which is suitable for high-silver ores.
4. Concentrate dehydration section
The lead-silver concentrate and zinc concentrate slurry are pumped into high-efficiency thickeners respectively for pre-concentration, and then sent to the disc filter for filtration; the moisture content of the filter cake is controlled at 10% to 14%, and then enters the concentrate shed for stacking for export; the overflow water from the thickener is returned to the system for recycling.
5. Tailings transportation section
The flotation tailings are pumped into a chamber filter press through a slurry pump for filtering, and then transported to the tailings storage for storage;
, Reduce the footprint of the tailings pond. Mineral processing wastewater is recycled in a closed circuit, and the return water utilization rate is ≥90%.
Crushing and Screening: PE250×400 jaw crusher, PEX150×750 jaw crusher, vibrating screen, vibrating feeder, belt conveyor
Grinding and Classification: MQG1530 grate-discharge ball mill, MQG1530 overflow-type ball mill, hydrocyclone cluster, slurry pump
Flotation: SF-series mechanically agitated flotation cells, reagent mixing tank
Dewatering: High-efficiency thickener (one unit each for lead and zinc circuits), chamber filter press, disc filter